Guides / Alloys

Machining Waspaloy and X-750: the heat alloys for parts that run hotter than 718

November 27, 2026

Waspaloy and X-750 machining comes up when a part has to carry load hotter than alloy 718 can handle, or keep a spring or bolt load at temperature. Both are gamma-prime alloys: their strength comes from particles that form during aging, and that strength makes them slower to cut than almost anything else in the nickel family. Waspaloy is the stronger and harder to machine of the two. X-750 is chosen for springs, seals and bolts where loads are more modest.

This guide covers when each alloy is used, how they behave under the tool, how the multi-step heat treatment fits into the machining plan and what to write on the drawing.

Temperatures and cycles are typical published values, rounded. The specification on your drawing always governs.

Where 718 stops and these alloys start

Alloy 718 is strong up to about 650°C (1200°F). Above that, its gamma double-prime particles coarsen and change, and strength falls quickly. Parts that run hotter need an alloy strengthened by gamma prime, which stays stable to higher temperatures.

Alloy 718 Alloy X-750 Waspaloy
UNS N07718 N07750 N07001
Strengthened by Gamma double prime Gamma prime Gamma prime, more of it
Typical load-bearing limit About 650°C (1200°F) About 650 to 700°C (1200 to 1300°F) About 870°C (1600°F) for less demanding parts
Common parts Shafts, rings, valve and tool parts Springs, bolts, seals Rings, cases, seals, fasteners
Machining effort, typical Very high when aged High Very high

X-750 is often specified for its resistance to relaxation: a spring or bolt in X-750 keeps more of its load after long exposure to heat. Waspaloy is specified for strength and creep resistance in the hot section of turbines, and for ground hardware that sees the same temperatures, such as test cell fixtures.

How gamma-prime alloys machine

The particles that keep these alloys strong at temperature also keep them strong at the cutting edge. The tool, not the workpiece, takes the heat and the load. Three things follow.

Low cutting speeds. Speeds are a fraction of those used on stainless steel and lower again for fully aged Waspaloy. Higher speeds shorten tool life so much that the part costs more, not less.

Notch and flank wear. The hardened skin and abrasive particles wear tools at the depth-of-cut line. Varying the depth of cut between passes spreads that wear along the edge. Many shops change tools on a schedule rather than waiting for a failure that could scrap a costly part.

Work hardening. As with all nickel alloys, a dull or rubbing tool hardens the surface. Every pass has to cut under the layer left by the last one, so feeds must never drop too low and dwells in the cut must be avoided.

Features that are cheap in steel become cost drivers here: small deep holes, small threads, long thin walls and fine surface finishes. Thread milling is often preferred to tapping in aged material, and a slightly larger thread where the design allows it saves real time.

Fitting the heat treatment into the plan

Both alloys take more than one heat treatment step, and the machining plan has to fit around them.

X-750

Specifications for X-750 choose between several cycles depending on whether strength or relaxation resistance matters most. One common route is an equalizing step at about 885°C (1625°F) for 24 hours, then aging at about 704°C (1300°F) for 20 hours. Spring and bolt specifications can call for different sequences.

Waspaloy

A typical Waspaloy cycle has three steps: a solution treatment at about 995 to 1040°C (1825 to 1900°F), a stabilizing hold at about 845°C (1550°F) for 4 hours and an aging hold at about 760°C (1400°F) for 16 hours. Rotating and static parts can carry different cycles.

The machining routes

There are three usual ways to combine machining and heat treatment:

  1. Cut from fully heat-treated stock. No movement after machining, but the slowest cutting. Common for small parts, fasteners and tight tolerances.
  2. Rough, heat treat, finish. Rough in the solution-treated condition, run the stabilize and age steps, then finish the critical features. Faster for most of the stock and full control of final size.
  3. Machine, then heat treat. Fastest cutting, but the part can move during aging. Only suits open tolerances.

The heat treatment page covers these routes for every age-hardened alloy, including 718.

Material and lead time

Waspaloy and X-750 are less common in stock than 718 and 625, and they are usually bought to aerospace material specifications such as AMS 5706 or AMS 5707 for Waspaloy bar and AMS 5667 for X-750 bar. Sizes outside the common range may need a mill run, which can add months. Ask on the RFQ which stock sizes are available, and whether a forging or a larger standard bar would bring the date in.

Material cost is also high. On small batches it can be the largest single line on the quote, so a near-net forging or a smaller stock size often pays for itself in both material and machining time.

What to put on the drawing

  • The alloy, the material specification and the condition at delivery.
  • The heat treatment cycle or the specification that defines it, and whether heat treatment may follow rough machining.
  • The hardness or tensile requirement, and where on the part or on which coupon it is tested.
  • Tolerances that reflect function. A general tolerance of ±0.005 in (±0.13 mm) on non-functional features is typical; save ±0.0005 in (±0.013 mm) for the features that need it.
  • Surface finish on the features where it matters, typical machined finishes being 63 to 32 µin Ra (1.6 to 0.8 µm).
  • Tests and documents: penetrant test, first article report, heat treatment certificate, mill certificate.

For the full picture of alloy choice by temperature and environment, see the Inconel machining guide by service condition. For how an order runs from RFQ to the document pack, see what to send and what you get with Inconel machining services.

To price a Waspaloy or X-750 part, send the drawing for a quote. We reply within 24 business hours with questions or a feasibility note.

Frequently asked questions

When is Waspaloy used instead of 718?

When the part carries load above about 650°C (1200°F), where alloy 718 loses strength quickly. Waspaloy keeps useful strength and creep resistance to about 870°C (1600°F) and is common for turbine rings, cases, seals and fasteners in that band.

Is X-750 easier to machine than Waspaloy?

Usually, yes. Both are age-hardened gamma-prime alloys, but X-750 has less of the strengthening phase and no cobalt, so it is somewhat less abrasive. Waspaloy, especially fully aged, is among the slowest alloys of the nickel family to machine.

Should Waspaloy be machined before or after aging?

It depends on the tolerances and the specification. Roughing in the solution-treated condition, then stabilizing, aging and finishing the critical features is a common route. Some specifications require the part to be cut from fully heat-treated stock. Write the allowed route on the drawing.